Common Problems And Solutions in The Use Of Thermal Insulation Plastics

May 19, 2025

Leave a message

    When thermal insulation plastics are used in industrial furnaces and other scenarios, various problems may occur due to material characteristics, improper construction or environmental factors. The following are common problems, cause analysis and solutions, I hope they will be helpful to you.

Serial number

Frequently asked questions

Problem manifestation

Cause Analysis

Workaround

1

Hollow, falling off

The insulation layer is separated from the kiln base, making a hollow sound when knocked, and in severe cases the entire layer may peel off.

1.There is dust, oil or old coating on the surface of the substrate, which leads to insufficient adhesion. The substrate is separated and makes a hollow sound when knocked. In severe cases, the whole piece will peel off.

2.The interface agent is not applied or is applied unevenly, especially on metal furnace walls or smooth surfaces, so the plastic and the substrate cannot "bite" each other.

3.If plastic is stored for too long, the binders (such as phosphates and clay) will become damp and deteriorate, and lose their stickiness.

1.Knock off the hollow parts, clean the base layer thoroughly with a wire brush and compressed air, and wipe the oily areas with alcohol or alkaline water.

2.Apply clay slurry or phosphate solution (mixed according to the material instructions) evenly on the cleaned base, and resume construction after drying.

3.If the material is expired or spoiled, replace it with fresh plastic directly to avoid making do with it.

2

Surface cracking

The appearance of a network of fine cracks or penetrating cracks on the surface of the insulation layer may cause heat leakage or structural damage.

1. The thickness of a single construction exceeds 50mm, the bottom material sinks due to its own weight, and the top shrinks and cracks

2.The surface is not covered to keep it moist after construction, or the ambient temperature is too high or the wind speed is too high, which causes the surface to lose water and shrink quickly.

3.The kiln heats up too quickly, causing uneven thermal expansion inside the insulation layer, or no expansion joints are left.

1. The thickness of each layer should be controlled at 30-50mm, and the upper layer should be constructed after the lower layer is compacted and hardened.

2.Cover with plastic sheet immediately after construction and maintain at room temperature for 24-48 hours, avoiding direct sunlight and strong wind.

3.Filling and leaving gaps: Small cracks (less than 2mm) can be repaired with plastic slurry; large cracks require the cracked parts to be removed and refilled, and 3-5mm expansion joints should be left every 2-3 meters.

3

Not compacted

The inside of the insulation layer is loose, there is a crisp sound when knocked, the thermal insulation performance is reduced, and it may even fall off partially.

1. The plastic material is too dry and hard (not enough material has been prepared or it has lost water due to long storage), and it cannot fit tightly when pounded.

2.The "cross" tamping method (alternating horizontal and vertical compaction) was not used, or the hammering force or frequency was insufficient.

3.Large-scale construction is done by manual ramming with wooden hammers, which is inefficient and difficult to compact the interior.

1. Take out the plastic material 24 hours in advance and let it rest. If it is too dry, add a binder (such as phosphate solution) in proportion to mix it into a "plasticine" state.

2. Use a pneumatic tamping hammer (for large areas) or a rubber hammer (for small areas) to cross-tamp horizontally and then vertically until the surface is slurry and there is no depression.

3. Insert a steel needle. If there is strong resistance and no sticky material after pulling it out, it means it has been compacted.

4. Directly add or remove and refill the loose parts to ensure that there is no "false pressure" phenomenon.

4

Hardens slowly or does not harden

The paint has not solidified more than 48 hours after construction, and there are obvious dents when pressed by hand.

1. Randomly adjust the amount of 1.water or binder on site to destroy the chemical reaction conditions of the material.

2.During construction, the ambient temperature is less than 10°C and the curing reaction of the binder is slow.

3.Plastic has exceeded its shelf life and the binder has become ineffective.

1. Add the binder strictly according to the material instructions, and do not add water to dilute without authorization.

2. During winter construction, raise the ambient temperature to 15-25℃ and keep the temperature stable during maintenance.

3. After confirming that the material is expired, stop using it immediately and replace it with new material to avoid affecting the overall project quality.

5

Thermal insulation performance does not meet the standard

The surface temperature of the kiln is too high when it is running, energy consumption increases, or the thickness of the insulation layer does not meet the design requirements.

1. When using low-temperature plastic in high-temperature kilns, the material shrinks and the pores increase under high temperatures.

2.The construction was not carried out in layers according to the designed thickness, or the compression ratio was not enough during tamping.

1. Select the corresponding material according to the maximum temperature of the kiln.

2. For areas with insufficient thickness, add a layer of plastic after the base layer is solidified to ensure that the total thickness meets the design requirements.