Maintenance After Initial Setting
Start Time
The initial setting of the surface of the corundum mullite castable begins immediately, usually 4 to 6 hours at room temperature after construction.
Maintenance Methods
Cover and retain moisture: Cover the surface with plastic film, wet straw bags or conservation felt, ensuring complete coverage without omissions to prevent moisture evaporation.
Spray water for moisturizing: If the environment is dry (humidity <50%), spray water regularly to keep the surface moist. The spraying frequency should be such that there is condensation water on the inside of the film to avoid direct flushing that may cause sand on the surface.
Ambient Temperature Requirements
Normal temperature curing (15~25℃): Natural curing, no additional heating or cooling required.
Low temperature environment (5~15℃): Cover with a quilt or build a greenhouse. If necessary, mix the material with hot water (water temperature ≤60℃) to delay the initial setting time.
High temperature environment (>25℃): Avoid direct sunlight, set up a sunshade, and increase the frequency of water spraying to once every 2 hours to prevent surface cracking.
Hardening And Curing
The curing period of corundum mullite castable is generally 3~7 days (adjusted according to the type of binder). Aluminate cement bonding requires at least 3 days of curing to ensure that calcium aluminate hydrate is fully formed. The curing period of phosphate bonding can be extended to 5~7 days, and a slightly acidic environment must be maintained (avoid contact with alkaline substances).
Drying And Baking
The purpose of drying and baking is to gradually remove moisture to avoid sudden temperature rise that causes excessive internal steam pressure and causes explosion, while promoting the stability of the material's crystal form.
|
Temperature Range |
Heating Rate |
Insulation Time |
Target |
|
normal temperature~150℃ |
10~15℃/h |
8~12 h |
Removal of free water |
|
150~300℃ |
15~20℃/h |
6~8 h |
Removal of crystal water |
|
300℃~Operating temperature |
At design rate |
2~4 h |
Adapt to working temperature and stabilize structure |
Note: It is strictly forbidden to heat directly from room temperature to high temperature. The temperature must be raised in stages. After each stage, wait for the temperature in the furnace to be uniform. Large equipment needs to set up multiple temperature measurement points to ensure that the temperature rises synchronously in all parts, and the temperature difference is ≤50℃. If cracks are found during the drying process, the temperature must be stopped immediately, the insulation time must be extended, or the temperature must be slowly lowered before re-baking.
Through the above scientific and reasonable maintenance, the corundum mullite castable can form a uniform and dense structure, maximize its high temperature resistance, corrosion resistance, wear resistance and other characteristics, and ensure long-term and reliable service in industrial kilns.