Heat-resistant Steel Parts for Furnaces

Heat-resistant Steel Parts for Furnaces

Heat resistant steel refers to alloy steel that has high strength and good chemical stability at high temperatures. Anti oxidation steel generally requires good chemical stability, but can withstand lower loads. Hot strength steel requires high high-temperature strength and corresponding oxidation resistance. Heat resistant steel is commonly used to manufacture components that work at high temperatures in industrial sectors such as boilers, steam turbines, power machinery, industrial furnaces, aviation, and petrochemicals. These components not only require high temperature strength and resistance to high temperature oxidation and corrosion, but also require sufficient toughness, good processability and weldability, as well as a certain degree of organizational stability according to their different uses.
Heat resistant steel for industrial furnaces: In addition to reactors, power plant boilers, and petrochemical industrial furnaces, it is widely used in metallurgy, machinery, building materials, light industry, and other industries as various heat-resistant components in various furnaces such as heat exchangers, heating furnace tubes, and reaction tanks. In addition to using heat-resistant steel deformation materials such as plates, tubes, and rods, a large number of heat-resistant steel castings are also used. Various annealing furnace covers in metallurgical plants, muffle tanks, radiation tubes, loading frames, chain belts, etc. for controllable gas continuous heating furnaces are mostly made of 310 (0Cr25Ni20) or 3Cr24Ni7SiNRe, 2Cr25Ni13 steel, etc.
Send Inquiry
Description
product-800-800

A large number of furnace bottom rollers and radiation tubes in continuous heating furnaces and heat treatment furnaces in metallurgical plants are also made of high alloy heat-resistant steel centrifugal cast pipes. Commonly used grades include 0Cr18Ni9, 00Cr18Ni9, 1Cr18Ni9Ti, 0Cr17Ni12Mo2, 00Cr17Ni12Mo2, 3Cr24Ni7SiNRe, 0Cr23Ni13, 1Cr20Ni14, Cr25Ni20Si2, 00Cr10Ni20Mo6Cu6, 4Cr25Ni35NbW, 70CrMoVBRe, 4Cr28Ni48W5Si2, 3Cr26Ni4MnMoRe, etc.

In the cement industry, a large number of heat-resistant steel components such as 3Cr24Ni7SiNRe, 1Cr20Ni14, Cr25Ni20Si2, etc. are used in the preheating belt of wet cement kilns, the grate plate used in large cement inspection and cooling machines, and the material hopper used in cooling machines

 

Heat-resistant steel parts for furnaces and kilns

 

Stainless steel grade correspondence table:

 

Commonly used austenitic stainless steel, heat-resistant steel and austenitic-ferritic stainless steel grades and their chemical compositions

No.

Chinese Brand GB/T20878-2007

Main chemical components

 

Unified digital code

Old brand

New grades

Ni

Cr

C

Si

Mn

P

S

Mo

N

Ti

1

304

0Cr18Ni9

 

8.00-11.00

17.00-19.00

≤0.08

≤1.00

≤2.00

≤0.035

≤0.03

--

--

--

     

08Cr19Ni10

8.00-11.00

18.00-20.00

≤0.08

≤1.00

≤2.00

≤0.045

≤0.03

--

--

--

2

309s

0Cr23Ni13

 

12.00-15.00

22.00-24.00

≤0.08

≤1.00

≤2.00

≤0.035

≤0.03

--

--

--

     

06Cr23Ni13

12.00-15,00

22.00-24.00

≤0.08

≤1.00

≤2.00

≤0.045

≤0.03

--

--

--

3

310s

0Cr25Ni20

 

19.00-22.00

24.00-26.00

≤0.08

≤1.00

≤2.00

≤0.035

≤0.03

--

--

--

     

06Cr25Ni20

19.00-22.00

24.00-28.00

≤0.08

≤1.50

≤2.00

≤0.045

≤0.03

--

--

--

4

316L

00Cr17Ni14Mo2

 

12.00-15.00

16.00-18.00

≤0.03

≤1.00

≤2.00

≤0.035

≤0.03

2.00-3.00

--

--

     

022Cr17Ni12Mo2

10.00-14.00

18.00-18.00

≤0.03

≤1.00

≤2.00

≤0.045

≤0.03

2.00-3.00

--

--

5

321

1Cr1BNi9Ti

 

8.00-11.00

17.00-19.00

≤0.12

≤1.00

≤2.00

≤0.035

≤0.03

--

--

Ti≥5(C%-0.02)

     

08Cr18Ni11Ti

9.00-12.00

17.00-19.00

≤0.08

≤1.00

≤2.00

≤0.045

≤0.03

--

--

Ti≥5(C%-0.02)

6

2205

 

022Cr23Ni5Mo3N

4.50-6.50

22.00-23.00

≤0.03

≤1.00

≤2.00

≤0.03

≤0.02

3.00-3.50

0.14-0.20

--

Table of commonly used martensitic steel grades and their chemical compositions

No.

Chinese Brand GB/T20878-2007

Main chemical components

 

Unified digital code

Old brand

New grades

Ni

Cr

C

Si

Mn

P

S

Mo

N

Ti

1

0Cr13

0Cr13

 

--

11.50-13.00

≤0.08

≤1.00

≤1.00

≤0.035

≤0.03

--

--

--

     

08Cr13

0.6

11.50-13.50

≤0.08

≤1.00

≤1.00

≤0.04

≤0.03

--

--

--

2

1Cr13

1Cr13

 

--

11.50-13.50

≤0.15

≤1.00

≤1.00

≤0.035

≤0.03

--

--

--

     

12Cr13

0.6

12.00-14.00

≤0.15

≤1.00

≤1.00

≤0.04

≤0.03

--

--

--

3

2Cr13

2Cr13

 

--

2.00-14.00

0.16-0.25

≤1.00

≤1.00

≤0.035

≤0.03

--

--

--

     

20Cr13

0.6

12.00-14.00

0.15-0.25

≤1.00

≤1.00

≤0.04

≤0.03

--

--

--

4

3Cr13

3Cr13

 

--

12.00-14.00

0.26-0.35

≤1.00

≤1.00

≤0.035

≤0.03

--

--

--

     

30Cr13

0.6

12.00-14.00

0.25-0.35

≤1.00

≤1.00

≤0.04

≤0.03

--

--

--

Hot Tags: heat-resistant steel parts for furnaces, China heat-resistant steel parts for furnaces manufacturers, suppliers, factory, Low Cement Bond Chemical Bond No burn Precast, High Strength Lightweight Refractory Brick, Micro expanding Refractory Plastic, Anchor, YXJ Acid resistant and Heat resistant Elastic Sealant For Power Plants, Refractory Concrete Precast Blocks